Open Problems

Tractable Open

How do particles bond in cold spray?

In cold spray, metal powder fired at supersonic speed sticks to a surface without melting. Whether bonding needs a shear instability at the interface or comes from pressure-driven jetting is disputed.

coatingsadditive manufacturingimpact mechanicsmaterials

On this page
  1. The problem
  2. Why it matters
  3. What counts as progress
  4. Known approaches
  5. Dead ends
  6. References
  7. Related problems
  8. Attempts (0)

The problem

Cold spray accelerates metal particles, typically 5 to 50 micrometres across, in a supersonic gas jet. Above a material-dependent critical velocity the particles stick to the substrate and to each other, building up coatings or whole parts, all without melting. The process is used for repairs, corrosion coatings and solid-state additive manufacturing.

The long-standing explanation is adiabatic shear instability: at impact, intense local heating softens the metal at the interface faster than it hardens, producing a jet of material that strips oxide and brings clean metal into contact. Single-particle impact experiments and simulations have since argued that the jetting is driven instead by a pressure wave released at the contact edge, and that shear instability is not needed. The two views predict the critical velocity differently and suggest different ways to improve bonding.

Why it matters

The critical velocity sets which materials can be sprayed, the gas and equipment cost, and the strength of the deposit. A settled mechanism would let engineers predict it for new alloys and powders instead of finding it by trial.

What counts as progress

  • Single-particle impact experiments with controlled velocity and temperature that measure bonding and interfacial structure for several metals, published with the raw data.
  • A model that predicts the critical velocity for alloys not used to fit it, within a stated error, compared against these measurements.
  • Direct observation, for example by time-resolved imaging or post-impact microscopy, that distinguishes the signatures each mechanism predicts.
  • An account of the role of surface oxide thickness, tested by varying it deliberately.

Known approaches

Laser-induced projectile impact tests on single particles; finite element and molecular dynamics simulations of impact; transmission electron microscopy of bonded interfaces; empirical critical-velocity formulas fitted to spray trials.

Dead ends

Simulations whose result depends on mesh size, or on the choice of material model at extreme strain rates, cannot by themselves settle the mechanism. Empirical critical-velocity fits that work for the alloys they were trained on are not evidence for either mechanism.

References

  1. Assadi et al. (2003): Bonding mechanism in cold gas spraying
  2. Hassani-Gangaraj et al. (2018): Adiabatic shear instability is not necessary for adhesion in cold spray
  3. Wikipedia: Cold spraying